Silicone vs EPDM vs NBR vs FKM: How to Select Elastomer Material for Custom Molded Seals and Gaskets

Choosing elastomer for a custom molded seal, gasket, O-ring or diaphragm is rarely hardness-only. The wrong polymer passes incoming inspection, then reappears as leaks, swelling, hardening, cracking, set or odor/taste complaints. Balance continuous and peak temperature, fluids, chemicals, compression set, regulatory path, geometry limits and price. No elastomer wins every axis, so specify from the operating envelope, not habit.

The Four Elastomer Families at a Glance

Silicone has a siloxane backbone, the widest temperature span, excellent ozone/UV/weathering, low compression-set potential and clean food/medical options, but modest tear/abrasion and poor aromatic oil or fuel resistance. EPDM excels in heat, ozone, steam, hot water, brake fluid and glycol coolant, yet swells in mineral oils and fuels. NBR is the value oil/fuel workhorse at moderate temperature, fair in abrasion, weak in ozone/weathering unless protected. FKM gives extreme heat and aggressive fuel/chemical resistance with low swell, at premium cost and reduced low-temperature flexibility.

Typical traitSiliconeEPDMNBRFKM
Continuous service, typical-60 to +200 C; selected to +230 C-50 to +150 C-40 to +120 C; low-temp grades lower-20 to +200 C; specialty beyond
Low-temperature flexibilityExcellentGood to very goodFair; compound dependentLimited unless specialty
Oil and fuel resistancePoor to fairPoor in hydrocarbonsGood to very goodExcellent
Ozone and weatheringExcellentExcellentPoor unless protectedExcellent
Steam and hot waterGoodExcellentPoor to fairFair; grade dependent
Compression set behaviorTypically lowCompound dependentCompound dependentTypically low
Relative costMedium to highLow to mediumLowHigh to premium

Property Comparison with Engineering Numbers

Treat published bands as screening values, not guarantees. Confirm compounds against ASTM D2000 callouts where used; measure hardness by ASTM D2240, tension by ASTM D412, compression set by ASTM D395 and fluid response by ASTM D471. Geometry, flash, knit lines, fillers, post-baking and test conditions move results.

Property and common methodSiliconeEPDMNBRFKM
Hardness span, Shore A typical30 to 8040 to 9040 to 9060 to 90
Tensile, ASTM D412, MPa typical4 to 108 to 188 to 208 to 16
Tear strength, kN/m typical8 to 2520 to 4525 to 6015 to 40
Compression set, ASTM D395 typicalOften low; 10 to 30 percent at stated conditionCompound dependent; 15 to 45 percentCompound dependent; 15 to 50 percentOften low; 10 to 30 percent
IRM 903 oil response, ASTM D471High swell; unsuitableHigh swell; unsuitableLow to moderate swellVery low swell
Fuel or aromatic exposurePoorPoorGood for many fuelsExcellent

For sealing, durometer is only the surface story. A 70 Shore A part can still extrude under pressure, take set at temperature or tear during installation; request the data sheet, test condition and permissible change limits.

Industry Fit: Where Each Elastomer Wins

Match the polymer to dominant exposure, then verify secondary fluids. Medical, baby and healthcare parts often favor silicone where ISO 10993 biocompatibility and FDA 21 CFR 177.2600 food limits are in the release package; see medical silicone parts. High-cavity precision parts may use LSR injection molding when justified.

Application environmentPrimary fitWhy it winsCommon caution
Medical, baby, healthcare, food contactSiliconeWide temperature, cleanliness, low odor and taste potentialConfirm ISO 10993 or FDA path per product
Automotive under-hood and fuelFKM; NBR for value; EPDM for coolant and brake fluidHeat, fuel, oil or polar fluid separationNever put EPDM in hydrocarbon oil service
Outdoor glazing, construction, HVACEPDM or siliconeOzone, UV and weathering decide lifeMind tear strength at thin lips
Appliance, hot water, potable waterEPDM or siliconeSteam, hot water and aging stabilityVerify local potable-water approval needs
Hydraulic and general oil sealingNBRBest price-performance in many hydrocarbon fluidsAvoid ozone-rich outdoor exposure

Use field complaints as re-selection triggers. Swelling signals fluid mismatch, hardening oxidation or heat age, cracking ozone or flex fatigue, permanent set compression set at temperature, and color/taste issues contamination or wrong family. A hardness tweak rarely fixes chemistry.

From Material Choice to Molded Part: Design and RFQ Checklist

Send enough data for DFM and material review before cutting steel.

  1. Define operating envelope: minimum/maximum continuous temperature, peak excursions, pressure, fluids/chemicals with concentrations, duty cycle and storage.
  2. State environment: indoor/outdoor, ozone, UV, washdown chemicals, steam, salt fog, cleaning cycles and assembly lubricants.
  3. Declare regulatory path: ISO 10993 for medical contact, FDA 21 CFR 177.2600 or EU 1935/2004 for food contact, potable-water needs, and flame/automotive standards.
  4. Specify hardness by ASTM D2240 target/tolerance, plus tension, tear, elongation and abrasion by ASTM D412 or equivalent.
  5. Set compression set by ASTM D395 with temperature, time, specimen and maximum percent change; state post-fluid-aging needs.
  6. Flag geometry drivers: thin walls, undercuts, flash limits, parting-line location, tolerances, bond inserts, tear-prone lips and inspection access.
  7. Give annual volume, launch timing, cavity-count logic, tooling ownership, revision control and prototype/bridge/multi-cavity needs.
  8. List deliverables: material data sheet, dimensional report, first article inspection, certificates of conformance, and PPAP/customer-specific documents where automotive applies.
RFQ data requiredMinimum detail to provide
Drawing and CADCurrent revision, critical dimensions, tolerances, sealing surfaces
ExposureTemperature profile, fluids with concentration, pressure, ozone and UV
ComplianceISO 10993, food contact, potable water, flame or PPAP scope
CommercialAnnual volume, target price, delivery region, packaging and inspection level

Frequently Asked Questions

Is silicone always better than NBR and EPDM for seals and gaskets?

No. Silicone works well around -60 to +200 C with strong ozone/weathering, but poorly in aromatic fuels/oils. NBR suits hydrocarbon oil at moderate temperature; EPDM suits steam, hot water, coolant and brake fluid.

Which elastomer is best for oil and fuel resistance at moderate cost?

NBR is the moderate-cost baseline for oil/fuel near -40 to +120 C, with specialty low-temperature grades. Move to FKM near +200 C continuous heat, aggressive fuels or tight ASTM D471 swell limits.

Can World Strong Rubber mold all four elastomers in custom geometries?

World Strong Rubber molds custom silicone, EPDM, NBR and FKM with in-house tooling and ISO 9001/ISO 13485 quality systems. Suitability still depends on compound, drawing, tolerances and validated tests, not family name alone.

Conclusion

The best elastomer is the one whose weakest property still clears your worst real exposure. Send World Strong Rubber your conditions, fluid list with concentrations, drawings/CAD, target hardness, regulatory path and volumes for DFM and material review. With in-house tooling, ISO 9001/ISO 13485 quality and disciplined control, aim for a manufacturable part matched to evidence, not universal performance.