LSR Mold Ejection and Demolding System Design for Soft Silicone Parts: A Buyer Guide
Demolding causes most torn parts, dimensional scrap and cycle-time loss in soft LSR molding. At 30-50 Shore A, silicone grips cores, stretches and springs back instead of sliding like rigid plastic, so pointed ejector pins puncture it. Choose the ejection strategy during mold design and use it to frame DFM questions before steel is cut.
Why Soft LSR Parts Are Hard to Demold
Soft LSR raises ejection force because several effects act together:
- Low hardness and high friction. At 30-50 Shore A the tacky surface deforms locally instead of transmitting push force.
- Elastic stretch and memory. Elongation at break is typically 300-700%, so the part wraps undercuts and pin tips.
- Vacuum adhesion. A soft part seals to a polished core; release may require breaking partial vacuum first.
- Undercuts and thin walls. Sealing lips, bellows and snap features lock onto cores while thin sections tear.
- Cure state and temperature. Hot or under-cured parts are weaker and tackier, so demolding temperature and post-cure schedule change release.
- Pin load concentration. A small pin applies the full load to a few square millimeters.
| Factor | Sticking effect | Design response |
|---|---|---|
| Shore A 30-50 | High tack and local deformation | Stripper plates or air ejection |
| Elongation 300-700% | Stretches over undercuts | Stripper rings, collapsible cores, split cavities |
| Polished core | Vacuum adhesion, no air path | Air blast, poppet valves, vent grooves |
| Undercuts / negative draft | Mechanical lock on core | Side actions, floating cores, two-stage ejection |
| Thin walls / hot cure state | Tear or stick under point loads | Uniform contact; stable temperature and validated cure |
Ejection System Options for LSR Molds
LSR molds use distributed contact, air or core movement rather than pins. Select the method at DFM with quality control planning for tear and flash criteria.
| Method | Contact | Best fit | Advantage | Limit |
|---|---|---|---|---|
| Stripper plate / ring | Large-area push | Thin cylindrical symmetric seals | Even load, no puncture | Needs gripping edge; plate cost |
| Air blast / poppet valve | None | Tacky optical and medical parts | Breaks vacuum, zero marking | Needs clean dry air; part may fly |
| Sleeve ejector | Annular push | Bosses, tubes, core-pin parts | Pushes strongest section | Round features only; sleeve wear |
| Two-stage / sequential | Air/lifter then stripper | Deep-drawn vacuum-prone parts | Low peak force | More complex controls |
| Collapsible / floating core | Core retracts | Internal undercuts, threads, grooves | Releases locked geometry | Highest cost and maintenance |
Ejection force depends on contact area, core draft, surface finish, ejection temperature and undercut depth. A stripper on a 40 Shore A seal can need far less force than pins because load spreads across the full edge.
Draft Angles, Surface Finish and Coatings for Release
Draft is the cheapest release feature. Use 1-2 degrees (typical) on cores and 0.5-1 degree (typical) on cavities. Zero or negative draft needs strip-over geometry, a collapsible core, split cavity or side action.
SPI A-level polish lowers interlock but can increase vacuum adhesion on conforming silicone; fine texture or EDM breaks suction and often releases tacky parts better. Hard chrome or Ni-PTFE reduce adhesion and wear without spray contamination. Avoid external spray release in medical and optical production because residues contaminate cleanrooms, interfere with bonding, printing and coating, and complicate ISO 13485 validation.
| Finish / treatment | Release effect | Application | Caution |
|---|---|---|---|
| High polish (SPI A) | Low interlock, possible vacuum adhesion | Optical and sealing surfaces | Pair with air ejection or venting |
| Fine texture / EDM | Breaks suction | Keypads, grips, general seals | Higher friction; cosmetic limits |
| Hard chrome | Lower adhesion, high wear resistance | High-volume cores/cavities | Thickness affects critical dimensions |
| Ni-PTFE composite | Low surface energy, durable release | Sticky low-durometer parts | Verify functional compatibility |
| Spray mold release | Effective but contaminating | Non-critical industrial only | Not for medical/optical lines |
Undercut Design Rules and the Buyer Demolding DFM/RFQ Checklist
Small external undercuts can strip over a ring when interference is low relative to 300-700% (typical) elongation and walls will not tear. Internal undercuts, deep grooves and threads usually need collapsible cores, split cavities or side actions. Gate and cold-runner design must keep vestiges off sealing surfaces and avoid stretching the part across the gate. For flash-free cleanroom production, robotic pick-and-place with vision check gives consistent removal, no operator contact and documented certifications support.
- State Shore A hardness, geometry and annual volume.
- List every undercut and negative-draft feature with dimensions and depth.
- Call out wall thickness, thin lips and no-touch sealing zones.
- Specify allowed draft or where zero draft is mandatory.
- Define permitted finishes and coatings on functional surfaces.
- Declare cleanroom/medical requirements, including no spray release.
- Ask the mold maker to propose and justify the ejection method.
- Set cycle-time and automation targets, including robotic handling.
- Define allowed gate and vestige locations.
- Agree inspection, tear and scrap acceptance criteria before tooling.
| RFQ data required | Why needed |
|---|---|
| Shore A, drawing, 3D model | Selects ejection method and draft strategy |
| Undercut list with dimensions | Decides strip-over vs collapsible core or side action |
| Cleanroom / medical class | Rules out sprays; defines air ejection and handling |
| Volume and cycle target | Sizes automation, cavities and cooling |
| Acceptance criteria | Aligns tear, flash and vestige limits with QC |
Frequently Asked Questions
Why cannot ordinary ejector pins be used to demold soft 30 Shore A silicone parts?
At 30 Shore A the silicone is soft and tacky, so a pointed pin concentrates the full ejection load on a few square millimeters and punctures or dimples the part. Stripper plates, air blast or poppet valves spread the load or avoid contact.
What draft angle should I specify on an LSR mold for a soft silicone seal?
A typical starting point is 1-2 degrees on cores and 0.5-1 degree on cavities, marked typical rather than guaranteed. Zero or negative draft is possible but needs strip-over design, collapsible cores or side actions, so flag it early.
Is spray mold release acceptable for medical-grade silicone production?
Generally no. Spray residues contaminate cleanrooms, interfere with post-bonding and printing, and complicate ISO 13485 validation. Permanent treatments such as Ni-PTFE or hard chrome, combined with air ejection, are preferred.
Conclusion
Send us your part drawings, undercut details, Shore A hardness and production volume for a demolding DFM review and ejection-system proposal. World Strong Rubber builds LSR tooling in-house in Dongguan under ISO 9001 and ISO 13485 certified quality systems, with 28 years of experience in soft silicone parts and documented quality control at every stage.
Related: custom mold making · LSR injection molding · equipment and capacity