LSR Mold Gate Design for Custom Silicone Parts: Gate Types, Sizing Rules and Buyer Questions

In liquid silicone rubber (LSR) injection molding, the gate is where material enters the cavity — and it is the single feature that most directly decides part quality. A poorly designed gate leaves visible vestige, flash, knit lines or uncured sections on custom molded silicone parts such as seals, gaskets, O-rings, valves, bellows and medical components. A well-designed gate delivers clean auto-degating, uniform cure and consistent dimensions shot after shot. This guide explains the four gate types used in LSR tooling, the concrete sizing rules our engineers apply, and the questions OEM buyers should ask any LSR mold maker before issuing a PO.

Why Gate Design Matters in LSR Molding

LSR has a viscosity of roughly 500–5000 Pa·s at injection temperature, is injected at 80–200 bar, and cures in the mold at 170–200 °C in 30–180 seconds depending on wall thickness (typically 1–4 mm). Because LSR is a thermoset, material that cures inside the gate or runner is scrap — you cannot regrind and reuse it. The gate therefore controls fill pattern, shear rate, air evacuation, cure uniformity and the size of the mark left on the finished part. Most cosmetic and functional complaints we see on transferred tools trace back to gate decisions made before steel was cut.

DefectGate-related causeGate-related fix
Flash at parting line or gateFilm gate land too thick (over 0.5 mm) or worn shut-offRestore land to 0.2–0.5 mm; re-machine or shim the gate plate
Gate vestige on sealing facePin gate placed on a functional surfaceRelocate gate; hold vestige ≤0.1 mm on sealing surfaces
Knit (weld) lines in sealsSingle point gate on annular geometry; flow fronts meetSwitch to ring gate for concentric, knit-free filling
Short shots in thin sectionsUndersized pin gate restricts high-viscosity LSROpen gate toward 1.0 mm; verify pressure margin in the 80–200 bar window
Burn marks (diesel effect)Air trapped at dead-end filling by poor gate positionMove gate to last-fill location; add venting at the flow front

The Four Gate Types and When to Use Each

LSR molds use four gate families. The right choice depends on part geometry, sealing function, cavitation and how the part will be removed from the runner.

Gate typeTypical partVestigeCavitation fit
Pin (point) gate, 0.4–1.0 mmSmall seals, valves, medical components0.05–0.15 mm bump; auto-degates by tear strength at demoldingLow to medium cavitation
Film (flash) gate, land 0.2–0.5 mmThin-wall gaskets, diaphragms, bellowsMinimal flash line; risk of flash if land wearsLow cavitation, wide or flat parts
Ring gateO-rings, face seals, annular gasketsConcentric ring vestige; removed by trimming or tear-degatingMedium cavitation
Valve gate (cold runner)High-volume O-rings, medical componentsPin-point vestige with positive shut-off; fully automatic degatingHigh cavitation, 16–128 cavities

For parts in Shore A 30–70, pin and valve gates degate cleanly because LSR’s tear strength lets the runner pull away from a small-diameter gate without tearing the part.

Gate Sizing and Location Rules

Our mold designers follow six rules on every LSR tool. Use them to review any gate layout proposed for your parts:

  1. Gate into the thickest wall section. For walls of 1–4 mm, place the gate at the thickest area so material flows toward thinner sections; this packs the cavity fully before cure slows flow. Cure time scales from about 30 seconds at 1 mm to 180 seconds at 4 mm.
  2. Keep gates off sealing surfaces. Target vestige height of 0.05–0.15 mm is acceptable on non-critical faces, but must be ≤0.1 mm — ideally zero — on static or dynamic sealing surfaces. If geometry forces the gate near a seal, gate onto a sacrificial tab instead.
  3. Size pin gates to the viscosity window. A 0.4–1.0 mm pin gate works with LSR viscosity of 500–5000 Pa·s. Exploit shear thinning at the gate — shear rate drops viscosity during injection — but avoid going so small that jetting, burn marks or short shots appear.
  4. Balance multi-cavity runners. Every cavity must fill at equal pressure within the 80–200 bar injection window. Use flow simulation and, on cold runner tools, machine runner branches to equal length and diameter so all cavities cure identically at 170–200 °C.
  5. Actively cool the cold runner plate. Insulated or water-cooled runner plates keep LSR in the runner below cure temperature while the cavity runs hot. This eliminates runner scrap entirely — critical for medical and high-cavitation production.
  6. Design the vestige direction and degating method up front. Decide whether parts tear off at the pin gate, get punched, or drop automatically from valve gates, and confirm the vestige direction matches your assembly and inspection drawings.

Buyer Checklist: Gate Questions to Ask Your LSR Mold Maker

Gate quality is where tooling claims get tested. Ask these questions before signing a PO — a capable supplier answers all of them with numbers, not generalities.

QuestionGood answer
Who designs the gate layout?In-house tooling engineers using mold-flow simulation, with LSR-specific gate libraries — not copied from thermoplastic tools
Do you build and maintain molds in-house?Yes — in-house custom mold making with in-house repair, so gate wear (a film gate land, for example) is fixed in days, not months
How is gate vestige verified?CMM measurement at the gate, with ±0.05 mm capability on critical sealing dimensions, documented through formal quality control records
Does the FAI report cover the gate area?Yes — first article inspection includes vestige height, degating quality and seal-surface readings at the gate location
Cold runner or valve gate for my cavitation?Insulated/actively cooled cold runner with pin gates up to ~16 cavities; valve gates for higher cavitation — both give zero runner scrap
What mold life and gate maintenance do you expect?1M+ shots with scheduled gate-plate inspection; insert-style gates for low-cost replacement

FAQ

What is a typical gate vestige on an LSR molded part?

Typical pin gate vestige height is 0.05–0.15 mm. On sealing surfaces the requirement is stricter — ≤0.1 mm — and on critical sealing dimensions we hold ±0.05 mm by CMM measurement. Valve gates with positive shut-off produce the smallest, most consistent mark.

Which gate type is best for silicone O-rings and gaskets?

Use a ring gate for O-rings and annular face seals: it fills concentrically and eliminates knit lines that become leak paths. For thin flat gaskets, a film (flash) gate with a 0.2–0.5 mm land gives near-zero vestige. High-volume O-ring production benefits from valve gates in a cold runner for automatic degating.

Do LSR molds use hot runners or cold runners?

LSR molds use cold runners — insulated or actively cooled plates that keep material in the runner below cure temperature while cavities run at 170–200 °C. Unlike thermoplastic hot runners, this gives zero runner scrap, which matters because cured silicone cannot be reprocessed. Valve gates on the cold runner are the standard choice for high cavitation.

Conclusion

Gate design is where LSR part quality is won or lost. Pin, film, ring and valve gates each have a defined role, and the sizing rules — 0.4–1.0 mm pin gates, 0.2–0.5 mm film lands, vestige ≤0.1 mm on seals — are concrete enough that buyers should demand them by name. At World Strong Rubber, our 28 years of ISO 9001 / ISO 13485 production and in-house mold design and making mean gate decisions are made by the same engineers who will build, sample and maintain your tool.

Send us your drawings or 3D models and we will return a DFM review that flags gate location, vestige risk and degating method on every critical feature — before you commit to steel. Request your quote today.

Related: custom mold making · quality control · LSR injection molding · factory tour

✉️ Get a Quote 💬 WhatsApp 📞 +86 180 0288 9642